{"id":7869,"date":"2023-06-28T09:56:27","date_gmt":"2023-06-28T01:56:27","guid":{"rendered":"https:\/\/uetpcb.com\/?p=7869"},"modified":"2023-06-28T10:27:09","modified_gmt":"2023-06-28T02:27:09","slug":"bga-solder-joints","status":"publish","type":"post","link":"https:\/\/uetpcb.com\/fr\/bga-solder-joints\/","title":{"rendered":"Analyse des d\u00e9fauts et am\u00e9lioration du processus des joints de soudure BGA"},"content":{"rendered":"<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"878qd-0-0\">\n<div data-offset-key=\"878qd-0-0\">Nous aborderons les crit\u00e8res d'acceptation, les caract\u00e9ristiques des d\u00e9fauts et la fiabilit\u00e9 des joints de soudure des BGA. Nous proc\u00e9derons notamment \u00e0 une analyse plus approfondie d'un d\u00e9faut controvers\u00e9 : les vides. Nous proposerons \u00e9galement quelques am\u00e9liorations de processus visant \u00e0 optimiser la qualit\u00e9 des joints de soudure des BGA.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"878qd-0-0\"><\/div>\n<div data-offset-key=\"878qd-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"fd0b-0-0\">\n<h2 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fd0b-0-0\"><span data-offset-key=\"fd0b-0-0\">1. Introduction au BGA<\/span><\/h2>\n<\/div>\n<\/div>\n<\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<p>&nbsp;<\/p>\n<p>Le BGA est un composant conditionn\u00e9 selon la technologie \u00ab ball grid array \u00bb (grille de billes). Il est apparu au d\u00e9but des ann\u00e9es 1990. \u00c0 cette \u00e9poque, en raison du nombre croissant de broches des composants dans les bo\u00eetiers \u00e0 broches, l'espacement entre les broches ne cessait de diminuer, ce qui a conduit \u00e0 un espacement minimal de 0,3 mm (12 mils). En termes d'assemblage, cette situation avait atteint les limites en mati\u00e8re de fabricabilit\u00e9 et de fiabilit\u00e9 du soudage des composants. Cela entra\u00eenait un risque accru d'erreurs. C'est alors qu'est apparu un nouveau type de composant en bo\u00eetier BGA (Ball Grid Array). Par rapport aux composants QFP de m\u00eame taille, le BGA peut offrir un nombre de broches plusieurs fois sup\u00e9rieur.<br \/>\nDans le cas d'un BGA, les billes de soudure situ\u00e9es sous la puce remplacent les broches. L'espacement entre les broches est relativement important, ce qui facilite l'assemblage. Cela permet d'am\u00e9liorer consid\u00e9rablement le taux de conformit\u00e9 des soudures et le taux de r\u00e9ussite d\u00e8s la premi\u00e8re tentative.<\/p>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<p>Le PBGA, g\u00e9n\u00e9ralement conditionn\u00e9 dans du plastique, est le composant le plus couramment utilis\u00e9 dans les produits de communication et les produits grand public. La composition de ses billes de soudure est g\u00e9n\u00e9ralement un alliage eutectique 63n\/37Pb. Les composants CBGA en bo\u00eetier c\u00e9ramique sont parfois utilis\u00e9s dans les produits militaires, et leurs billes de soudure sont constitu\u00e9es d\u2019un alliage non eutectique \u00e0 haute temp\u00e9rature de type 10Pb\/90Sn. Avec le d\u00e9veloppement continu des composants BGA, les \u00c9tats-Unis et le Japon ont mis au point des BGA miniatures dot\u00e9s de bo\u00eetiers plus petits, dont la taille n\u2019est que de 20 % sup\u00e9rieure \u00e0 celle de la puce.<\/p>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\"><span style=\"font-size: 14.4px;\" data-offset-key=\"87bal-7-0\">G\u00e9n\u00e9ralement appel\u00e9s \u03bcBGA (microBGA) ou CSP. <\/span><span class=\"hardreadability\" style=\"font-size: 14.4px;\"><span data-offset-key=\"87bal-8-0\">Leurs billes de soudure ont atteint une <\/span><\/span><span class=\"complexword\" style=\"font-size: 14.4px;\"><span data-offset-key=\"87bal-9-0\">minimum<\/span><\/span><span class=\"hardreadability\" style=\"font-size: 14.4px;\"><span data-offset-key=\"87bal-10-0\"> de 0,3 mm (12 mil), et l'espacement entre les billes de soudure a atteint une <\/span><\/span><span class=\"complexword\" style=\"font-size: 14.4px;\"><span data-offset-key=\"87bal-11-0\">minimum<\/span><\/span><span class=\"hardreadability\" style=\"font-size: 14.4px;\"><span data-offset-key=\"87bal-12-0\"> de 0,5 mm (12 mil)<\/span><\/span><span style=\"font-size: 14.4px;\" data-offset-key=\"87bal-13-0\">. <\/span><span class=\"hardreadability\" style=\"font-size: 14.4px;\"><span data-offset-key=\"87bal-14-0\">En effet, pour les fabricants de circuits imprim\u00e9s, la r\u00e9alisation de vias entre des billes de soudure aussi rapproch\u00e9es constitue un d\u00e9fi majeur<\/span><\/span><span style=\"font-size: 14.4px;\" data-offset-key=\"87bal-15-0\"><span style=\"font-size: 14.4px;\" data-offset-key=\"87bal-15-0\">. Un travail tr\u00e8s difficile.<\/span><\/span><\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div data-offset-key=\"5mhn8-0-0\"><\/div>\n<\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<p><img decoding=\"async\" class=\"wp-image-7873 aligncenter\" src=\"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/bga_pcb-300x196.webp\" alt=\"bga_pcb\" width=\"466\" height=\"304\" srcset=\"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/bga_pcb-300x196.webp 300w, https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/bga_pcb.webp 555w\" sizes=\"(max-width: 466px) 100vw, 466px\" \/><\/p>\n<h2>2. Contr\u00f4le de la qualit\u00e9 des soudures des BGA<\/h2>\n<\/div>\n<\/div>\n<\/div>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Le contr\u00f4le de la qualit\u00e9 des soudures BGA est difficile, car les billes de soudure se trouvent sous la puce. En l\u2019absence d\u2019\u00e9quipement de contr\u00f4le, v\u00e9rifiez visuellement si l\u2019anneau de soudure le plus ext\u00e9rieur est r\u00e9gulier et examinez la puce \u00e0 contre-jour. Si chaque ligne et chaque colonne laisse passer la lumi\u00e8re, on peut en conclure qu\u2019il n\u2019y a pas de soudure continue. Parfois, on peut \u00e9galement observer des points de soudure de plus grande taille. Afin d\u2019\u00e9valuer plus pr\u00e9cis\u00e9ment la qualit\u00e9 des joints de soudure, il est \u00e9galement n\u00e9cessaire d\u2019utiliser un appareil d\u2019inspection aux rayons X.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Les \u00e9quipements traditionnels de radiographie directe bidimensionnelle par rayons X sont relativement peu co\u00fbteux. Ils pr\u00e9sentent toutefois un inconv\u00e9nient : les soudures situ\u00e9es des deux c\u00f4t\u00e9s du circuit imprim\u00e9 apparaissent simultan\u00e9ment sur une m\u00eame image. Lorsque des composants sont pr\u00e9sents des deux c\u00f4t\u00e9s au m\u00eame emplacement, leurs ombres de soudure se chevauchent. Il est alors difficile de distinguer le c\u00f4t\u00e9 du composant. En cas de d\u00e9faut, il est impossible de d\u00e9terminer clairement quelle couche est concern\u00e9e. Il est donc impossible de r\u00e9pondre \u00e0 l\u2019exigence de d\u00e9tection pr\u00e9cise des d\u00e9fauts de soudure.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Notre inspecteur de circuits imprim\u00e9s par rayons X est un \u00e9quipement d\u2019inspection tomographique par rayons X sp\u00e9cialement con\u00e7u pour contr\u00f4ler les joints de soudure. Bien entendu, il permet non seulement de contr\u00f4ler les BGA, mais aussi les joints de soudure de tous les composants pr\u00e9sents sur le circuit imprim\u00e9. Auparavant, on estimait que ce type d\u2019\u00e9quipement \u00e9tait trop co\u00fbteux et que le co\u00fbt de l\u2019inspection des joints de soudure \u00e9tait trop \u00e9lev\u00e9. Cependant, avec la g\u00e9n\u00e9ralisation croissante des dispositifs BGA, ce mat\u00e9riel on\u00e9reux a fini par \u00eatre accept\u00e9.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">X-Ray utilise la tomographie par rayons X. Gr\u00e2ce \u00e0 cette technique, les billes de soudure peuvent \u00eatre superpos\u00e9es, cr\u00e9ant ainsi un effet tomographique. Les images de tomographie par rayons X permettent d'analyser automatiquement les joints de soudure en fonction des donn\u00e9es de conception originales de CDA et des param\u00e8tres d\u00e9finis par l'utilisateur. Il effectue un balayage tomographique en temps r\u00e9el et peut comparer et analyser avec pr\u00e9cision tous les joints de soudure de tous les composants situ\u00e9s sur les deux faces du circuit imprim\u00e9 en quelques dizaines de secondes ou en 2 minutes (selon le nombre et la complexit\u00e9 des joints de soudure pr\u00e9sents sur le circuit). Il permet ainsi de d\u00e9terminer si la soudure est conforme ou non. Pourquoi la radiographie tomographique permet-elle d\u2019obtenir des r\u00e9sultats en tr\u00e8s haute d\u00e9finition ? Cela tient \u00e0 son principe de fonctionnement.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Les rayons X du syst\u00e8me sont g\u00e9n\u00e9r\u00e9s par un tube \u00e0 rayons X situ\u00e9 \u00e0 l'extr\u00e9mit\u00e9 sup\u00e9rieure de l'appareil. En fonctionnement, la tension doit \u00eatre port\u00e9e de 220 V \u00e0 160 kV, et le courant est de 100 mA. Des faisceaux d'\u00e9lectrons g\u00e9n\u00e9r\u00e9s \u00e0 haute tension irradient du tungst\u00e8ne m\u00e9tallique pour produire des rayons X. Ce faisceau de rayons X est projet\u00e9 obliquement vers le bas et tourne \u00e0 une vitesse \u00e9lev\u00e9e de 760 tours par seconde. Parall\u00e8lement, une plate-forme \u00e0 scintillateur situ\u00e9e en dessous tourne \u00e9galement de mani\u00e8re synchrone avec le faisceau de rayons X, \u00e0 la m\u00eame vitesse.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">\n<p>La plate-forme \u00e0 scintillateur est en r\u00e9alit\u00e9 un r\u00e9cepteur sensible aux rayons X. De mani\u00e8re g\u00e9n\u00e9rale, les m\u00e9taux, notamment les m\u00e9taux lourds tels que l\u2019\u00e9tain et le plomb, ne laissent pas passer les rayons X et forment une image sombre. La mati\u00e8re ordinaire est travers\u00e9e par les rayons X, et rien n\u2019est alors visible. Les rayons X sont rassembl\u00e9s en un point pr\u00e9cis situ\u00e9 entre la source lumineuse et la plate-forme \u00e0 scintillateur, ce qui d\u00e9finit un plan de focalisation. Les objets ou images situ\u00e9s sur ce plan de focalisation forment une image nette sur la plate-forme \u00e0 scintillateur. En revanche, les objets ou images qui ne se trouvent pas sur ce plan de focalisation apparaissent flous sur la plate-forme \u00e0 scintillateur, ne laissant qu\u2019une ombre.<\/p>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">\n<p>&nbsp;<\/p>\n<p>Le principe de la tomographie par rayons X est illustr\u00e9 sur la figure. La tomographie est donc r\u00e9alis\u00e9e sur des joints de soudure pr\u00e9sentant diff\u00e9rentes hauteurs sur le circuit imprim\u00e9. Si vous souhaitez v\u00e9rifier l'\u00e9tat de soudure d'une couche donn\u00e9e, il vous suffit d'aligner cette couche sur la position du plan de focalisation, et les r\u00e9sultats du balayage s'afficheront clairement. Cette image nette sera captur\u00e9e par une cam\u00e9ra \u00e0 rayons X situ\u00e9e sous le dispositif.<\/p>\n<\/div>\n<p><img decoding=\"async\" class=\"wp-image-7874 aligncenter\" src=\"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga-300x231.webp\" alt=\"pcb_bga\" width=\"435\" height=\"335\" srcset=\"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga-300x231.webp 300w, https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga.webp 592w\" sizes=\"(max-width: 435px) 100vw, 435px\" \/><\/p>\n<h2 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">3. Crit\u00e8res d'acceptation des joints de soudure des BGA<\/h2>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Quel que soit l'\u00e9quipement d'inspection utilis\u00e9, il doit exister une base permettant de d\u00e9terminer si la qualit\u00e9 des joints de soudure est conforme. La norme IPC-A-610C d\u00e9finit pr\u00e9cis\u00e9ment les crit\u00e8res d'acceptation des joints de soudure des BGA. Les joints de soudure BGA doivent pr\u00e9senter les caract\u00e9ristiques suivantes : ils doivent \u00eatre lisses, ronds, avec des contours nets et ne comporter aucun vide. Le diam\u00e8tre, le volume, la nuance de gris et le contraste de tous les joints de soudure doivent \u00eatre identiques ; leur position doit \u00eatre align\u00e9e, sans d\u00e9calage ni torsion, et aucune boule de soudure ne doit \u00eatre pr\u00e9sente.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Une fois l'op\u00e9ration termin\u00e9e, la norme recommand\u00e9e est appliqu\u00e9e, mais de mani\u00e8re l\u00e9g\u00e8rement assouplie pour les soudures conformes. Pour les positions align\u00e9es, la soudure BGA peut pr\u00e9senter un d\u00e9calage ne d\u00e9passant pas 25 % par rapport au plot. La bille de soudure ne doit pas d\u00e9passer 25 % de la distance entre les billes de soudure les plus proches.<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h2 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">4. D\u00e9fauts courants des joints de soudure des BGA<\/h2>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Les d\u00e9fauts typiques des BGA comprennent : les joints de soudure, les circuits ouverts, les billes de soudure manquantes, les vides importants, les billes de soudure trop grosses et les bords irr\u00e9guliers des joints de soudure. Vous trouverez ci-dessous une liste de radiographies issues de cas r\u00e9els, illustrant la plupart des d\u00e9fauts mentionn\u00e9s ci-dessus.<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<h2 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">5. Un vice de forme controvers\u00e9 \u2013 nullit\u00e9<\/h2>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Une question qui fait encore l'objet de d\u00e9bats concerne les crit\u00e8res d'acceptation des vides dans les BGA. Le probl\u00e8me des vides n'est pas propre aux BGA. Les joints de soudure des composants \u00e0 trous traversants et \u00e0 montage en surface peuvent g\u00e9n\u00e9ralement faire l'objet d'une inspection visuelle pour d\u00e9tecter d'\u00e9ventuels vides, plut\u00f4t que d'une inspection par rayons X. Dans les BGA, comme tous les joints de soudure sont cach\u00e9s sous le bo\u00eetier, ils ne peuvent \u00eatre inspect\u00e9s qu\u2019aux rayons X. Bien s\u00fbr, les rayons X peuvent \u00eatre utilis\u00e9s pour inspecter non seulement les joints de soudure des BGA, mais aussi tous les types de joints de soudure. Gr\u00e2ce aux rayons X, les vides peuvent \u00eatre facilement d\u00e9tect\u00e9s.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Le vide aurait-il donc un impact n\u00e9gatif sur la fiabilit\u00e9 du BGA ? Ce n'est pas certain. Certains vont m\u00eame jusqu'\u00e0 affirmer que la formation de vides est b\u00e9n\u00e9fique pour la fiabilit\u00e9. La norme IPC-7095, intitul\u00e9e \u2018 Processus de conception et d'assemblage pour la r\u00e9alisation de BGA \u2019, fournit des directives d\u00e9taill\u00e9es concernant la conception des BGA et les technologies d'assemblage. Le comit\u00e9 IPC-7095 reconna\u00eet que de petites cavit\u00e9s in\u00e9vitables peuvent \u00eatre b\u00e9n\u00e9fiques pour la fiabilit\u00e9. Cependant, il devrait exister une norme d\u00e9finie permettant de d\u00e9terminer la taille acceptable de ces cavit\u00e9s.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">5.1 Emplacement et cause du vide<\/h3>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">O\u00f9 peut-on d\u00e9tecter des vides lors de l'inspection des joints de soudure d'un BGA ? Les billes de soudure d'un BGA peuvent \u00eatre divis\u00e9es en trois couches : la couche du composant (substrat proche du composant BGA), la couche du pad (substrat proche du circuit imprim\u00e9) et la couche interm\u00e9diaire de la bille de soudure. Selon les circonstances, des vides peuvent appara\u00eetre dans n'importe laquelle de ces trois couches.<\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Quand ces vides sont-ils apparus ? Les billes de soudure des BGA peuvent elles-m\u00eames contenir des vides avant le soudage, ce qui entra\u00eene la formation de vides une fois le processus de soudage par refusion termin\u00e9. Cela peut \u00eatre d\u00fb \u00e0 l'introduction de vides lors du processus de fabrication des billes de soudure, ou \u00e0 un probl\u00e8me li\u00e9 \u00e0 la p\u00e2te \u00e0 souder appliqu\u00e9e sur la surface du circuit imprim\u00e9. Par ailleurs, la conception du circuit imprim\u00e9 est \u00e9galement une cause majeure de formation de vides.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Par exemple, si le trou de via est con\u00e7u sous le plot, lors du processus de soudage, l'air ext\u00e9rieur p\u00e9n\u00e8tre dans la bille de soudure fondue par le trou de via, ce qui laisse une cavit\u00e9 dans la bille de soudure une fois le soudage termin\u00e9 et le refroidissement effectu\u00e9.<\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Les vides pr\u00e9sents dans la couche de pastille peuvent \u00eatre dus \u00e0 la volatilisation du flux contenu dans la p\u00e2te \u00e0 souder d\u00e9pos\u00e9e sur la pastille lors du processus de soudage par refusion ; le gaz s'\u00e9chappe alors de la soudure lors de la p\u00e9n\u00e9tration en profondeur, et les vides se forment apr\u00e8s refroidissement. Un placage de mauvaise qualit\u00e9 ou une contamination de la surface du plot peuvent \u00e9galement \u00eatre \u00e0 l'origine de vides dans la couche de plot.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">La couche de composants est souvent la zone la plus susceptible de pr\u00e9senter des vides, situ\u00e9e entre le centre de la bille de soudure et le substrat du BGA. Cela peut \u00eatre d\u00fb \u00e0 la pr\u00e9sence de bulles d\u2019air et de gaz de flux volatilis\u00e9 sur le plot du BGA lors du soudage par refusion sur le circuit imprim\u00e9. Un vide se forme lors de la soudure. Si la courbe de temp\u00e9rature de refusion n'est pas suffisamment longue dans la zone de refusion, les bulles d'air et les gaz volatilis\u00e9s contenus dans le flux n'ont pas le temps de s'\u00e9chapper, et la soudure fondue p\u00e9n\u00e8tre dans la zone de refroidissement o\u00f9 elle se solidifie, formant ainsi une cavit\u00e9.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Par cons\u00e9quent, le profil de temp\u00e9rature de refusion est \u00e0 l'origine de la formation de vides. Les BGA utilisant un alliage de soudure eutectique 63N\/37Pb sont les plus susceptibles de pr\u00e9senter des vides, tandis que les BGA compos\u00e9s de billes de soudure ill\u00e9gales eutectiques \u00e0 haut point de fusion 10Sn\/90Pb, dont le point de fusion est de 302 \u00b0C, ne pr\u00e9sentent g\u00e9n\u00e9ralement pas de vides. Les billes de soudure du BGA ne fondent pas pendant le processus de soudage par refusion.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">5.2 Crit\u00e8res d'acceptation nuls<\/h3>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">La pr\u00e9sence de gaz dans la cavit\u00e9 peut entra\u00eener des contraintes de retrait et de dilatation lors des cycles thermiques. L'emplacement de la cavit\u00e9 deviendra un point de concentration des contraintes et pourra \u00eatre \u00e0 l'origine de fissures de contrainte.<br \/>\nCependant, la pr\u00e9sence de vides r\u00e9duit la contrainte m\u00e9canique exerc\u00e9e sur les billes de soudure en diminuant l'espace exc\u00e9dentaire qu'elles occupent. L'ampleur de cette r\u00e9duction d\u00e9pend de la taille, de l'emplacement, de la forme et d'autres facteurs li\u00e9s \u00e0 la cavit\u00e9.<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Les crit\u00e8res d'acceptation\/de rejet des vides sp\u00e9cifi\u00e9s dans la norme IPC-7095 prennent principalement en compte deux aspects : la position et la taille des vides. Peu importe o\u00f9 se trouve le vide, que ce soit au centre de la bille de soudure, dans la couche de pastilles ou dans la couche de composants, sa taille et sa quantit\u00e9 auront une incidence sur la qualit\u00e9 et la fiabilit\u00e9. De petits vides sont autoris\u00e9s \u00e0 l'int\u00e9rieur des billes de soudure. Le rapport entre l\u2019espace occup\u00e9 par le vide et l\u2019espace de la bille de soudure peut \u00eatre calcul\u00e9 comme suit : par exemple, si le diam\u00e8tre du vide repr\u00e9sente 50 % du diam\u00e8tre de la bille de soudure, alors la surface occup\u00e9e par le vide correspond \u00e0 25 % de la surface de la bille de soudure.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">La norme IPC stipule que les vides pr\u00e9sents dans la couche de pastilles ne doivent pas d\u00e9passer 10 % de la surface des billes de soudure. Les vides sup\u00e9rieurs \u00e0 25 % sont consid\u00e9r\u00e9s comme des d\u00e9fauts, pr\u00e9sentant des risques pour la fiabilit\u00e9 m\u00e9canique et \u00e9lectrique. Pour les vides compris entre 10 % et 25 %, il est recommand\u00e9 d'am\u00e9liorer le processus afin de les \u00e9liminer ou de les r\u00e9duire.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h2 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">6. Conclusion : suggestions d'am\u00e9lioration des processus visant \u00e0 r\u00e9duire les d\u00e9fauts des BGA<\/h2>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Lorsque la p\u00e2te \u00e0 souder eutectique (BGA) forme des joints de soudure au cours du processus de soudage, la p\u00e2te \u00e0 souder appliqu\u00e9e sur le circuit imprim\u00e9 et les billes de soudure contenues dans les composants doivent fusionner. Ce processus se divise en deux phases d\u2019effondrement. Au cours de la premi\u00e8re \u00e9tape, la p\u00e2te \u00e0 souder pr\u00e9sente sur le circuit imprim\u00e9 fond en premier, ce qui provoque l'affaissement des composants. Au cours de la deuxi\u00e8me \u00e9tape, les billes de soudure des composants eux-m\u00eames fondent \u00e9galement et fusionnent avec la p\u00e2te \u00e0 souder fondue sur le circuit imprim\u00e9 ; les billes de soudure s'affaissent \u00e0 nouveau, formant ainsi un joint de soudure aplati.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Pour r\u00e9aliser un joint de soudure parfait, il convient de pr\u00eater attention aux aspects suivants :<\/h3>\n<p>(1) Utilisez de la p\u00e2te \u00e0 souder fra\u00eeche afin de garantir qu'elle soit bien m\u00e9lang\u00e9e, que le d\u00e9p\u00f4t de p\u00e2te soit pr\u00e9cis et que le positionnement du composant soit correct.<\/p>\n<\/div>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">(2) Pour les PBGA conditionn\u00e9s sous film plastique, il convient de les faire s\u00e9cher \u00e0 100 \u00b0C pendant 6 \u00e0 8 heures avant le soudage ; il est pr\u00e9f\u00e9rable de proc\u00e9der \u00e0 cette op\u00e9ration sous azote.<\/h3>\n<\/div>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">(3) Le profil de temp\u00e9rature de refusion est un facteur tr\u00e8s important.<\/h3>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">\n<p>Au cours du processus de soudage, il est n\u00e9cessaire de veiller \u00e0 ce que la courbe de soudage pr\u00e9sente des transitions naturelles, afin que l'appareil soit chauff\u00e9 de mani\u00e8re homog\u00e8ne, en particulier dans la<\/p>\n<\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Dans la zone de soudure, il est n\u00e9cessaire de s'assurer que tous les joints de soudure sont enti\u00e8rement fondus. Si la temp\u00e9rature est insuffisante, des joints de soudure froids peuvent se former, entra\u00eenant des surfaces de soudure rugueuses ou une fusion incompl\u00e8te lors de la deuxi\u00e8me phase de refusion. Cela peut entra\u00eener des fissures entre la p\u00e2te \u00e0 souder \u00e0 la surface du circuit imprim\u00e9 et la soudure du composant, ce qui se traduit par une soudure virtuelle ou une soudure ouverte.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">(4) La quantit\u00e9 de p\u00e2te \u00e0 souder appliqu\u00e9e doit \u00eatre adapt\u00e9e.<\/h3>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">\n<p>La viscosit\u00e9 de la p\u00e2te \u00e0 souder permet de maintenir temporairement le composant en place et d'\u00e9viter la formation de ponts de soudure pendant la fusion. Pour les gabarits BGA, l'ouverture du point de soudure repr\u00e9sente g\u00e9n\u00e9ralement 70 \u00e0 80 % de la taille du plot, et l'\u00e9paisseur du gabarit est habituellement de 0,15 mm (6 mil).<\/p>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">(5) Lors de la conception des pastilles des BGA sur le circuit imprim\u00e9, les pastilles de tous les points de soudure doivent \u00eatre de taille identique.<\/h3>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">\n<p>Si certains circuits doivent \u00eatre con\u00e7us sous les pastilles, il convient \u00e9galement de trouver un fabricant de circuits imprim\u00e9s adapt\u00e9. Les pastilles doivent \u00eatre perc\u00e9es \u00e0 l'emplacement pr\u00e9vu, et tout agrandissement non autoris\u00e9 de celles-ci doit \u00eatre \u00e9vit\u00e9. En effet, le trou de passage ne peut pas \u00eatre perc\u00e9 trop petit. Par cons\u00e9quent, apr\u00e8s le soudage, la quantit\u00e9 d'\u00e9tain et la hauteur varieront entre les grandes et les petites pastilles, ce qui peut entra\u00eener un court-circuit ou un circuit ouvert.<\/p>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<h3 class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">(6) Par ailleurs, il convient de souligner un point concernant le probl\u00e8me du masque de soudure lors de la fabrication des circuits imprim\u00e9s.<\/h3>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">\n<p>Avant de souder un BGA, assurez-vous que le masque antisoudure autour du plot est conforme et que les vias sont recouverts d'un film barri\u00e8re. L'ajout d'un film antisoudure sur l'autre face du circuit imprim\u00e9 pendant la production est inefficace. Le film antisoudure a pour but d'emp\u00eacher la formation d'air et de vides pendant le soudage, ainsi que d'emp\u00eacher la soudure de s'\u00e9couler \u00e0 travers les trous traversants.<\/p>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">L'impression de la p\u00e2te \u00e0 souder sans retouche permet d'\u00e9viter tout exc\u00e8s de soudure et d'am\u00e9liorer la qualit\u00e9 du soudage. Les trous de passage \u00e9tant plaqu\u00e9s, un exc\u00e8s de soudure ou des probl\u00e8mes de soudage peuvent entra\u00eener des d\u00e9fauts de court-circuit virtuel et des courts-circuits. La retouche des BGA est une solution de dernier recours, car elle prend beaucoup de temps.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<h2 data-offset-key=\"fv90c-0-0\">Conclusion<\/h2>\n<div class=\"\" data-block=\"true\" data-editor=\"e9he\" data-offset-key=\"eabv5-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"eabv5-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"9c845\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"5mhn8-0-0\">\n<div class=\"\" data-block=\"true\" data-editor=\"3ps8o\" data-offset-key=\"fv90c-0-0\">\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div class=\"public-DraftStyleDefault-block public-DraftStyleDefault-ltr\" data-offset-key=\"fv90c-0-0\">Pour r\u00e9ussir le soudage d'un BGA, il faut disposer de billes de soudure adapt\u00e9es et d'outils de retouche appropri\u00e9s. La pose de billes pr\u00e9sente un faible taux de r\u00e9ussite et entra\u00eene un gaspillage de ressources. Les puces r\u00e9par\u00e9es subissent au moins quatre cycles de refusion, ce qui nuit \u00e0 leur fiabilit\u00e9. Il est donc important de bien se pr\u00e9parer avant de souder un BGA afin de minimiser les d\u00e9fauts et d'obtenir un taux de r\u00e9ussite \u00e9lev\u00e9. Notre objectif est d'\u00e9liminer les d\u00e9fauts sans avoir \u00e0 proc\u00e9der \u00e0 des r\u00e9parations.<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>\n<div data-offset-key=\"fv90c-0-0\"><\/div>","protected":false},"excerpt":{"rendered":"<p>Nous discuterons des crit\u00e8res d'acceptation, de la performance des d\u00e9fauts et de la fiabilit\u00e9 des joints de soudure BGA. En particulier, une analyse plus approfondie est effectu\u00e9e sur un d\u00e9faut controvers\u00e9, le vide. Nous proposons \u00e9galement quelques am\u00e9liorations de processus pour am\u00e9liorer la qualit\u00e9 des joints de soudure BGA. 1. Introduction au BGA Le BGA est un dispositif de type Chen \u00e0 grille \u00e0 billes. Il...<\/p>","protected":false},"author":6,"featured_media":7874,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[16],"tags":[],"class_list":["post-7869","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-news"],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v28.6 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>Defect Analysis and Process Improvement of BGA Solder Joints<\/title>\n<meta name=\"description\" content=\"BGA solder joints on PCB provide reliable connections between the component and the board, ensuring efficient electrical and mechanical performance.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/uetpcb.com\/fr\/bga-solder-joints\/\" \/>\n<meta property=\"og:locale\" content=\"fr_FR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Defect Analysis and Process Improvement of BGA Solder Joints\" \/>\n<meta property=\"og:description\" content=\"BGA solder joints on PCB provide reliable connections between the component and the board, ensuring efficient electrical and mechanical performance.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/uetpcb.com\/fr\/bga-solder-joints\/\" \/>\n<meta property=\"og:site_name\" content=\"UETPCB\" \/>\n<meta property=\"article:published_time\" content=\"2023-06-28T01:56:27+00:00\" \/>\n<meta property=\"article:modified_time\" content=\"2023-06-28T02:27:09+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga.webp\" \/>\n\t<meta property=\"og:image:width\" content=\"592\" \/>\n\t<meta property=\"og:image:height\" content=\"455\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/webp\" \/>\n<meta name=\"author\" content=\"zfp\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\u00c9crit par\" \/>\n\t<meta name=\"twitter:data1\" content=\"zfp\" \/>\n\t<meta name=\"twitter:label2\" content=\"Dur\u00e9e de lecture estim\u00e9e\" \/>\n\t<meta name=\"twitter:data2\" content=\"12 minutes\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"Article\",\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/\"},\"author\":{\"name\":\"zfp\",\"@id\":\"https:\\\/\\\/uetpcb.com\\\/#\\\/schema\\\/person\\\/34355dc7b8585db7603570610c803008\"},\"headline\":\"Defect Analysis and Process Improvement of BGA Solder Joints\",\"datePublished\":\"2023-06-28T01:56:27+00:00\",\"dateModified\":\"2023-06-28T02:27:09+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/\"},\"wordCount\":2511,\"image\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/uetpcb.com\\\/wp-content\\\/uploads\\\/2023\\\/06\\\/pcb_bga.webp\",\"articleSection\":[\"News\"],\"inLanguage\":\"fr-FR\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/\",\"url\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/\",\"name\":\"Defect Analysis and Process Improvement of BGA Solder Joints\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/uetpcb.com\\\/wp-content\\\/uploads\\\/2023\\\/06\\\/pcb_bga.webp\",\"datePublished\":\"2023-06-28T01:56:27+00:00\",\"dateModified\":\"2023-06-28T02:27:09+00:00\",\"author\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/#\\\/schema\\\/person\\\/34355dc7b8585db7603570610c803008\"},\"description\":\"BGA solder joints on PCB provide reliable connections between the component and the board, ensuring efficient electrical and mechanical performance.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/#breadcrumb\"},\"inLanguage\":\"fr-FR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"fr-FR\",\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/#primaryimage\",\"url\":\"https:\\\/\\\/uetpcb.com\\\/wp-content\\\/uploads\\\/2023\\\/06\\\/pcb_bga.webp\",\"contentUrl\":\"https:\\\/\\\/uetpcb.com\\\/wp-content\\\/uploads\\\/2023\\\/06\\\/pcb_bga.webp\",\"width\":592,\"height\":455,\"caption\":\"pcb_bga\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/uetpcb.com\\\/bga-solder-joints\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/uetpcb.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"News\",\"item\":\"https:\\\/\\\/uetpcb.com\\\/category\\\/news\\\/\"},{\"@type\":\"ListItem\",\"position\":3,\"name\":\"Defect Analysis and Process Improvement of BGA Solder Joints\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/uetpcb.com\\\/#website\",\"url\":\"https:\\\/\\\/uetpcb.com\\\/\",\"name\":\"UETPCB\",\"description\":\"\",\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/uetpcb.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"fr-FR\"},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/uetpcb.com\\\/#\\\/schema\\\/person\\\/34355dc7b8585db7603570610c803008\",\"name\":\"zfp\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"fr-FR\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/dddd7a7d7728264cc7a8800684fbb4e67e444dec78c3f5d15e261e7026bb585c?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/dddd7a7d7728264cc7a8800684fbb4e67e444dec78c3f5d15e261e7026bb585c?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/dddd7a7d7728264cc7a8800684fbb4e67e444dec78c3f5d15e261e7026bb585c?s=96&d=mm&r=g\",\"caption\":\"zfp\"}}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"Analyse des d\u00e9fauts et am\u00e9lioration du processus des joints de soudure BGA","description":"Les soudures BGA sur les circuits imprim\u00e9s assurent des connexions fiables entre le composant et la carte, garantissant ainsi des performances \u00e9lectriques et m\u00e9caniques optimales.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/uetpcb.com\/fr\/bga-solder-joints\/","og_locale":"fr_FR","og_type":"article","og_title":"Defect Analysis and Process Improvement of BGA Solder Joints","og_description":"BGA solder joints on PCB provide reliable connections between the component and the board, ensuring efficient electrical and mechanical performance.","og_url":"https:\/\/uetpcb.com\/fr\/bga-solder-joints\/","og_site_name":"UETPCB","article_published_time":"2023-06-28T01:56:27+00:00","article_modified_time":"2023-06-28T02:27:09+00:00","og_image":[{"width":592,"height":455,"url":"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga.webp","type":"image\/webp"}],"author":"zfp","twitter_card":"summary_large_image","twitter_misc":{"\u00c9crit par":"zfp","Dur\u00e9e de lecture estim\u00e9e":"12 minutes"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"Article","@id":"https:\/\/uetpcb.com\/bga-solder-joints\/#article","isPartOf":{"@id":"https:\/\/uetpcb.com\/bga-solder-joints\/"},"author":{"name":"zfp","@id":"https:\/\/uetpcb.com\/#\/schema\/person\/34355dc7b8585db7603570610c803008"},"headline":"Defect Analysis and Process Improvement of BGA Solder Joints","datePublished":"2023-06-28T01:56:27+00:00","dateModified":"2023-06-28T02:27:09+00:00","mainEntityOfPage":{"@id":"https:\/\/uetpcb.com\/bga-solder-joints\/"},"wordCount":2511,"image":{"@id":"https:\/\/uetpcb.com\/bga-solder-joints\/#primaryimage"},"thumbnailUrl":"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga.webp","articleSection":["News"],"inLanguage":"fr-FR"},{"@type":"WebPage","@id":"https:\/\/uetpcb.com\/bga-solder-joints\/","url":"https:\/\/uetpcb.com\/bga-solder-joints\/","name":"Analyse des d\u00e9fauts et am\u00e9lioration du processus des joints de soudure BGA","isPartOf":{"@id":"https:\/\/uetpcb.com\/#website"},"primaryImageOfPage":{"@id":"https:\/\/uetpcb.com\/bga-solder-joints\/#primaryimage"},"image":{"@id":"https:\/\/uetpcb.com\/bga-solder-joints\/#primaryimage"},"thumbnailUrl":"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga.webp","datePublished":"2023-06-28T01:56:27+00:00","dateModified":"2023-06-28T02:27:09+00:00","author":{"@id":"https:\/\/uetpcb.com\/#\/schema\/person\/34355dc7b8585db7603570610c803008"},"description":"Les soudures BGA sur les circuits imprim\u00e9s assurent des connexions fiables entre le composant et la carte, garantissant ainsi des performances \u00e9lectriques et m\u00e9caniques optimales.","breadcrumb":{"@id":"https:\/\/uetpcb.com\/bga-solder-joints\/#breadcrumb"},"inLanguage":"fr-FR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/uetpcb.com\/bga-solder-joints\/"]}]},{"@type":"ImageObject","inLanguage":"fr-FR","@id":"https:\/\/uetpcb.com\/bga-solder-joints\/#primaryimage","url":"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga.webp","contentUrl":"https:\/\/uetpcb.com\/wp-content\/uploads\/2023\/06\/pcb_bga.webp","width":592,"height":455,"caption":"pcb_bga"},{"@type":"BreadcrumbList","@id":"https:\/\/uetpcb.com\/bga-solder-joints\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/uetpcb.com\/"},{"@type":"ListItem","position":2,"name":"News","item":"https:\/\/uetpcb.com\/category\/news\/"},{"@type":"ListItem","position":3,"name":"Defect Analysis and Process Improvement of BGA Solder Joints"}]},{"@type":"WebSite","@id":"https:\/\/uetpcb.com\/#website","url":"https:\/\/uetpcb.com\/","name":"UETPCB","description":"","potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/uetpcb.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"fr-FR"},{"@type":"Person","@id":"https:\/\/uetpcb.com\/#\/schema\/person\/34355dc7b8585db7603570610c803008","name":"zfp","image":{"@type":"ImageObject","inLanguage":"fr-FR","@id":"https:\/\/secure.gravatar.com\/avatar\/dddd7a7d7728264cc7a8800684fbb4e67e444dec78c3f5d15e261e7026bb585c?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/dddd7a7d7728264cc7a8800684fbb4e67e444dec78c3f5d15e261e7026bb585c?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/dddd7a7d7728264cc7a8800684fbb4e67e444dec78c3f5d15e261e7026bb585c?s=96&d=mm&r=g","caption":"zfp"}}]}},"_links":{"self":[{"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/posts\/7869","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/users\/6"}],"replies":[{"embeddable":true,"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/comments?post=7869"}],"version-history":[{"count":11,"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/posts\/7869\/revisions"}],"predecessor-version":[{"id":7876,"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/posts\/7869\/revisions\/7876"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/media\/7874"}],"wp:attachment":[{"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/media?parent=7869"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/categories?post=7869"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/uetpcb.com\/fr\/wp-json\/wp\/v2\/tags?post=7869"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}